Disclosure: This post contains affiliate links and I will be compensated if you make a purchase after clicking through my links. Learn More
The short answer to why preheat before welding is crack control. Heating the steel first slows the cooling rate, gives hydrogen time to escape, and lowers the shrinkage stress that pulls a fresh weld apart.
Most hobby work on thin mild steel never needs it. Thick plate, high-carbon or alloy steel, cold shops and tightly restrained joints are a different story, and that’s where preheat saves a part.
We pulled the reasons, the thickness rules, the heating methods and the measuring rules from Lincoln Electric, Miller and TWI, so you can tell when your job needs heat and how much.
What Is Preheat in Welding?
Preheat is heating the base metal around the joint to a set minimum temperature before you strike the arc. The heat covers the whole joint area, past the spot where the bead starts.
Codes and procedures treat it as a number. A Welding Procedure Specification (WPS) usually lists a minimum and maximum preheat temperature and how long the part must stay at that heat, according to Miller.
Interpass temperature is the base metal temperature between the first and last passes. Lincoln Electric states that it cannot fall below the preheat temperature, so the heat you add at the start has to hold for the whole weld.

Credit: www.youtube.com
Why Preheat Before Welding: The 4 Main Reasons
You preheat before welding to slow cooling, drive out hydrogen and moisture, and cut shrinkage stress. Lincoln Electric lists four reasons, and each one targets a different way a weld cracks.
1. It Slows the Cooling Rate
A cold, thick plate pulls heat out of the weld fast. Fast cooling leaves a hard, brittle structure in the weld and the heat affected zone (HAZ).
Preheat shrinks the gap between the arc temperature and the base metal. The weld cools slower and ends up with a more ductile structure that resists cracking.
2. It Lets Hydrogen Escape
Hydrogen gets into the weld from moisture, oil, rust and damp filler metal. Trapped hydrogen causes cold cracking, which can show up hours after the weld looks fine.
Slower cooling gives hydrogen time to diffuse out of the steel. Miller adds that preheat drives surface moisture off the joint before welding starts, which cuts hydrogen at the source.
3. It Cuts Shrinkage Stress
Weld metal shrinks as it cools, and the surrounding plate resists that pull. A warm part expands with the weld and shrinks more evenly with it.
Lincoln Electric calls this especially important in highly restrained joints, where the parts can’t move to relieve the stress.
4. It Keeps Some Steels Above Their Brittle Range
Some steels turn brittle below a certain temperature. Preheat raises them above the point where brittle fracture would happen during fabrication.
Preheat can also help a weld meet required properties such as notch toughness, according to Lincoln Electric.
When Do You Need to Preheat?
Lincoln Electric notes that preheat usually is not required on low carbon steels less than 1 in. (25 mm) thick. Miller says shops commonly preheat steel or steel alloy pipe and plate 1 inch thick or more.
Thickness is only one input. Lincoln Electric lists these factors for deciding on preheat:
- Code requirements: AWS D1.1 and other codes set minimum preheat by steel group, thickness and process.
- Section thickness: thicker sections pull heat away faster.
- Base metal chemistry: more carbon and alloy means higher hardenability.
- Restraint: rigid joints build more shrinkage stress.
- Ambient temperature: a cold shop chills the part before and between passes.
- Filler metal hydrogen content: low-hydrogen electrodes lower the need for heat.
- Past cracking: a joint that cracked before is a clear sign to add preheat.
Miller names oil and gas, transmission pipelines, power plants, structural steel, mining, shipbuilding and heavy equipment as industries where preheat is routine.
How Carbon Equivalent Predicts Preheat Need
Carbon equivalent (CE) rolls a steel’s chemistry into one number. A higher CE means the HAZ hardens more easily, so the steel needs more preheat.
Lincoln Electric gives this formula, with each element in weight percent from the mill test report:
CE = C + (Mn + Si)/6 + (Cr + Mo + V)/5 + (Ni + Cu)/15
Here’s a worked example with two made-up chemistries, used only to show the math. Plug in the numbers from your own mill cert for a real job.
| Element (wt %) | Example Steel A | Example Steel B |
|---|---|---|
| C | 0.12 | 0.20 |
| Mn | 0.60 | 1.20 |
| Si | 0.20 | 0.30 |
| Cr + Mo + V | 0 | 0.15 |
| Ni + Cu | 0 | 0.30 |
| CE result | 0.25 | 0.50 |
Steel B has double the CE of Steel A. Extra carbon and manganese push the number up fast, and Steel B will call for a higher preheat at the same thickness.
AWS D1.1 includes two methods for setting preheat when no code table applies: HAZ hardness control and hydrogen control. Lincoln Electric says the hydrogen method is extremely useful for high strength, low-alloy steels but may be too conservative for carbon steels.
Typical Preheat Temperatures
There’s no single preheat number. The right value comes from your code, WPS or steel supplier, and it changes with grade, thickness and process.
Two sourced examples show the scale. Lincoln Electric cites a minimum prequalified preheat of 225°F (107°C) for A572 Grade 50 and A36 jumbo sections 4 to 5 in. thick, welded with low-hydrogen electrodes, under AWS D1.1-96 Table 3.2.
For butt splices in those same jumbo sections, Lincoln Electric points to 350°F (175°C) under AISC LRFD J2.8. Code minimums may not be enough for highly restrained connections.
Miller gives an example of a part held between 250°F and 400°F for 30 minutes before welding. Treat these values as examples, not settings for your job.
Going over the minimum is usually fine on carbon steels. Lincoln Electric says about 100°F (40°C) above the minimum is acceptable there.
Quenched and tempered (Q&T) steels are the exception. They need both a minimum and a maximum preheat, followed closely, because overheating can damage the HAZ.
How to Preheat Steel Before Welding
The best method depends on part thickness, part size and the equipment you have. Miller compares four common options.
| Method | How It Heats | Pros | Cons |
|---|---|---|---|
| Induction | Magnetic field creates eddy currents inside the metal | Setup often under 5 minutes, uniform heat | Higher upfront cost, wrapping takes training |
| Open flame (rosebud torch) | Fuel gas flame on the surface | Portable, uses common torch gear | Uneven, slow, ongoing fuel cost, needs a fire watch |
| Resistance | Electrically heated ceramic pads | Heats without an open flame | Setup can take an hour or more, broken pads cause hot and cold spots |
| Oven | Convection heat around the whole part | Uniform, good for batches and large parts | Oven may need several hours to heat up |
Lincoln Electric adds that small production assemblies suit a furnace, and large structural parts often use banks of torches, electric strip heaters, or induction or radiant heaters.
How to Measure Preheat Temperature
A torch can make the surface read hot when the steel below is still cold. Where and when you measure matters as much as the tool.
Miller lists temperature-indicating crayons, thermocouples, infrared thermometers and thermal imaging cameras. TWI also names contact thermometers.
Two common rules set the measuring distance:
| Rule | Measuring Distance From the Joint | Which Side |
|---|---|---|
| AWS D1.1 (per Lincoln Electric) | At least the thickness of the thickest member, never less than 3 in. (75 mm), in all directions | Heat the side opposite the weld, measure next to the joint |
| BS EN ISO 13916 (per TWI) | 4 times the thickness for parts under 50 mm (about 2 in.); at least 75 mm for thicker parts | Reverse side from the heat source |
Under the ISO rule, a 10 mm plate gets checked 40 mm from the groove edge. A 25 mm plate gets checked 100 mm out.
Check the steel temperature right before you strike the arc on each pass. That one habit keeps you inside both the preheat and interpass limits.
Preheat Safety Tips
Preheated steel can burn skin long after it stops glowing. Wear welding gloves, mark hot parts, and never test temperature with a bare hand.
- Clear flammables from the area before using a rosebud torch, and keep a fire watch as Miller advises for open flame.
- Heat only clean metal. Burning oil, paint or galvanizing gives off fumes, so ventilate and use fume extraction.
- Check that cylinders, hoses and regulators are in good condition before any torch heating.
- Follow the induction or resistance equipment maker’s manual for cable wrapping and electrical safety.
Frequently Asked Questions
Does Mild Steel Need Preheat Before Welding?
Usually not when it’s thin. Lincoln Electric says low carbon steel under 1 in. (25 mm) thick rarely needs preheat. Thicker sections, high restraint, a cold shop or damp filler metal can change that, so check your code or WPS before skipping it on heavy work.
What Happens If You Don’t Preheat Before Welding?
On steel that needs it, the weld cools too fast. That can leave a hard, brittle heat affected zone and trap hydrogen, which leads to cold cracks. These cracks may appear hours after welding, so a joint that passes a visual check can still fail later.
How Long Should You Preheat Steel Before Welding?
Heat until the required temperature holds at the measuring distance, deeper than the surface. Your WPS may set a hold time; Miller gives an example of 30 minutes. Induction setups often heat in minutes, and an oven can need several hours to reach temperature.
Can You Preheat Steel With a Propane Torch?
Yes, a fuel gas rosebud torch is one of the four common preheat methods Miller lists. It’s easy to set up, but heat is uneven and slow on thick parts. Move the flame across the joint, measure on the far side, and keep a fire watch nearby.
What Is the Difference Between Preheat and Interpass Temperature?
Preheat is the base metal temperature before the first pass. Interpass temperature is the base metal temperature between the first and last passes. Lincoln Electric states interpass temperature cannot fall below the preheat temperature, so you may need to reheat between passes on cold days.
Final Words
Preheat exists to stop cracks. It slows cooling, lets hydrogen escape, eases shrinkage stress and keeps some steels out of their brittle range.
Thin mild steel rarely needs it. Plate 1 in. and up, higher carbon equivalent steels, restrained joints and cold shops are where you reach for the torch or induction blanket.
Take your temperature from your code or WPS, measure it at the right distance on the far side, and check it again before every pass.