What Is Down Slope on a TIG Welder? Settings and Uses

Disclosure: This post contains affiliate links and I will be compensated if you make a purchase after clicking through my links. Learn More

What is down slope on a TIG welder? It is the timed ramp that lowers your welding current to a final current when you end a weld. The machine tapers the amps over the seconds you set, so the puddle shrinks and fills before the arc goes out.

Without that ramp, the arc cuts off at full heat. The big puddle freezes all at once and often leaves a crater, and craters can crack.

Below, we explain what the down slope setting does, how it works with 2T and 4T trigger modes, and how to dial it in on scrap before you weld a real part.

What Is Down Slope on a TIG Welder?

Down slope is the time it takes the welder to drop from your weld current to the end current. Kemppi’s MasterTig manual defines it as the time during which the welding current gradually decreases to the end current level. A setting of zero turns the function off.

Brands use different names for the same idea. You’ll see “down slope”, “downslope”, “slope down” or “slope time” on the panel. The current it ends at may be called final current, crater current or end amps.

How Down Slope Works at the End of a Weld

A TIG weld on a machine with slope controls runs through a short sequence. On a machine like the ESAB TIG 400i, each stage has its own setting.

  1. Pre-flow: shielding gas starts before the arc.
  2. Initial current and up slope: the arc starts low and ramps up to weld current.
  3. Weld current: the main amperage you set for the joint.
  4. Down slope: the current ramps down over the time you set.
  5. Final or crater current: the arc holds at a low level, then stops.
  6. Post-flow: gas keeps flowing to protect the hot tungsten and weld.

Down slope sits between the weld current and the final current. The longer the time, the slower the amps fall and the more time you have to add filler to the shrinking puddle.

Video thumbnail on TIG upslope and down slope settings on a TIG welder

Credit: www.youtube.com

Why Down Slope Matters: Craters and Crater Cracks

Miller Electric lists weld craters among the common TIG problems. Its guide says ending a weld too abruptly creates craters that can crack. The causes it names are cutting the power instantly, which cools the puddle too fast, and pulling the filler rod away too soon.

TWI, the UK welding institute, explains the same effect for crater pipes. Switching the current off makes a large weld pool solidify fast, and the shrinking metal leaves a hollow at the end. Its advice is to reduce the current step by step and add filler to make up for the shrinkage.

Down slope automates that taper. Miller notes that machines with a crater control feature reduce the current at the end of a weld for you. Keep feeding filler rod during the ramp so the crater fills flush with the bead.

Down Slope With 2T and 4T Trigger Modes

How you trigger down slope depends on the torch switch mode. Check your manual, because the exact behavior varies by brand and model.

2T Mode

In 2T, you hold the trigger as you weld and release it to stop. Everlast explains that once you release the switch, the torch cycles down to the preset final current and ends the arc on its own. Some Kemppi models let a quick press cut the ramp short.

4T Mode

In 4T, you press and release to start, then press again to end. On most Everlast units, pressing and holding the switch ramps the current down and holds a low arc until you let go. That hold at crater current gives you extra time to finish filling the crater.

Foot Pedal Welding

With a foot pedal, you control the amps with your foot, so you make the down slope yourself. Ease off the pedal slowly at the end of the bead and keep adding rod. Everlast points out that a foot pedal can’t solve every welding situation, and a torch switch with slope timers is handy where a pedal won’t fit.

Typical Down Slope and Crater Current Ranges

Machine ranges show how much control you get. These figures come from the makers’ manuals. Your own machine may differ.

SettingExample machineRange in the manual
Down slope timeESAB TIG 400i0 to 25 seconds
Up slope timeESAB TIG 400i0 to 15 seconds
Crater currentESAB TIG 400i10 A up to the weld current
Start/crater currentLincoln “T” type machines (manual IM738)10% of weld current on USA units (160 A gives 16 A)
Up slope timerLincoln “T” type machines (manual IM738)0.1, 0.5, 1 or 4 seconds

There is no single correct down slope time. The right value depends on the metal, its thickness, your weld current and how fast you add filler.

How to Set Down Slope on a TIG Welder

Time: about 15 minutes | Difficulty: easy | Tools: TIG welder with slope control, scrap of the same metal, filler rod.

Safety: wear your helmet, gloves and jacket for test beads too, and weld in a well-ventilated space to keep fumes away from your face.

Video thumbnail showing crater fill and initial current settings for TIG down slope

Credit: www.youtube.com

Step 1: Set Your Weld Current First

Pick the amperage for the joint and metal thickness. Our TIG amperage chart is a starting point.

Step 2: Set the Final Current Low

Set the final or crater current well below the weld current. The Lincoln manual uses 10% of weld current as the USA default, which is a simple reference point.

Step 3: Start With a Short Down Slope

Begin with a short time on the down slope knob. Run a bead on scrap and release the trigger at the end, feeding rod as the amps fall.

Step 4: Read the Crater and Adjust

Check the end of the bead. A dip or a crack line means the ramp is too short, so add time. A long tail of extra metal or a cold, ropey end means the ramp is too long.

Step 5: Repeat on the Real Joint Type

Test again on the same joint and position you’ll weld. Thin sheet, thick plate and aluminum often need different settings, so note what works for each.

Common Down Slope Mistakes to Avoid

  • Leaving down slope at zero, which ends the arc at full current.
  • Pulling the filler rod away as soon as the ramp starts.
  • Lifting the torch away during the ramp, which drops gas coverage.
  • Setting post-flow too short, so the hot tungsten and crater oxidize.
  • Copying a time from another machine without testing it on scrap.

Frequently Asked Questions

What does down slope do on a TIG welder?

Down slope lowers the welding current to a final current over a set time when you end the weld. The slow taper lets the puddle shrink and fill with rod before the arc stops. That helps prevent craters and crater cracks at the end of the bead.

Is down slope the same as crater fill?

They are closely linked. Down slope is the timed ramp from weld current to final current. Crater fill, crater current or end amps is the low current the ramp ends at. Together they fill the crater, and some brands group both settings under a crater control feature.

Do I need down slope if I use a foot pedal?

With a foot pedal, you taper the amps yourself by easing off the pedal at the end of the bead. Slope timers matter most when you weld with a torch switch. Check your manual, because each brand handles slope settings in pedal mode in its own way.

What happens if down slope is too long?

A down slope that is too long keeps the arc on after the crater is full. You can end up with a cold, built-up tail, extra heat in thin parts and wasted gas. Shorten the time in small steps until the bead ends flush with no dip.

What is the difference between up slope and down slope?

Up slope ramps the current up from a start level to your weld current at the beginning of a weld. Down slope does the reverse at the end, ramping down to the final current. Up slope gives a soft start, and down slope gives a filled, crack-free crater.

Final Words

Down slope is a small setting that fixes a common TIG defect. It tapers your amps at the end of the weld so the puddle fills and cools slowly, and that cuts the risk of crater cracks.

Set your weld current, keep the final current low, and adjust the down slope time on scrap until the crater ends flush. Keep feeding rod through the ramp, and your bead ends will look as good as the rest of the weld.

Scroll to Top